3003 H14 Aluminum Data

 

Aluminum Balance
Copper 0.05 - 0.2
Iron 0.7 max
Manganese 1 - 1.5
Remainder Each 0.05 max
Remainder Total 0.15 max
Silicon 0.6 max
Zinc 0.1 max

 

Density 0.0986 lb/in3
Hardness, Brinell 40
Tensile Strength 22000 psi
Tensile Yield Strength 21000 psi
Elongation at Break 16 %
Modulus of Elasticity 10000 ksi
Poisson's Ratio 0.33
Fatigue Strength 9000 psi
Shear Modulus 3630 ksi
Shear Strength 14000 psi
Electrical Resistivity 4.16e-006 ohm-cm
CTE, linear 68°F 12.9 μin/in-°F
CTE, linear 250°C 13.9 μin/in-°F
Specific Heat Capacity 0.213 BTU/lb-°F
Thermal Conductivity 1100 BTU-in/hr-ft2-°F
Melting Point 1190 - 1210 °F

 

 

<<