2024 T4 Aluminum Data

Aluminum Balance
Chromium 0.1 max
Copper 3.8 - 4.9
Iron 0.5 max
Magnesium 1.2 - 1.8
Manganese 0.3 - 0.9
Remainder Each 0.05 max
Remainder Total 0.15 max
Silicon 0.5 max
Zinc 0.25 max

 

Density 0.1 lb/in3
Hardness, Brinell 120
Tensile Strength 68000 psi
Tensile Yield Strength 47000 psi
Elongation at Break 20 %
Modulus of Elasticity 10600 ksi
Poisson's Ratio 0.33
Fatigue Strength 20000 psi
Shear Modulus 4060 ksi
Shear Strength 41000 psi
Electrical Resistivity 5.82e-006 ohm-cm
CTE, linear 68°F 12.9 μin/in-°F
CTE, linear 250°C 13.7 μin/in-°F
Specific Heat Capacity 0.209 BTU/lb-°F
Thermal Conductivity 840 BTU-in/hr-ft2-°F
Melting Point 935 - 1180 °F

 

 

<<